Alloy | Density approx. | Composition in % | Important tempers | Tensile Strength Rm N/mm2 | Yield Stress Rp0,2 N/mm2 | Elongation A % | Electr. conductivity MS/s | |
---|---|---|---|---|---|---|---|---|
CuNi10Fe1Mn DIN EN 12163 12420 12449 12451 1652 1653 | CW352H | 8,9 | Ni 9,0 - 11,0 Fe 1,0 - 2,0 Mn 0,5 - 1,0 Cu bal. | Bars M R280 Plates walzhart R300 | ≥ 280 ≥ 300 | ≥ 90 ≥ 120 | ≥ 30 ≥ 25 | |
Comparable Specifications:
| ||||||||
CuNi30Mn1Fe DIN EN 12163 12420 12449 12451 1652 1653 | CW354H | 8,9 | Ni 30,0 - 32,0 Fe 0,4 -1,0 Mn 0,5 - 1,5 Cu bal. | Bars M R340 R420 Plates walzhart R320 | * ≥ 340 ≥ 420 * ≥ 320 | * ≥ 120 ≥ 180 * ≥ 120 | * ≥ 30 ≥ 14 * ≥ 30 | * * |
Comparable Specifications:
| ||||||||
CuNi14Al3 nicht in DIN/ DIN EN genormt | 2.1504 | 8,5 | Ni 13,0 - 16,0 Al 2,0 - 3,0 Cu bal. | Richtwerte | ≥ 780 | ≥ 590 | ≥ 10 | ? |
High-strength, corrosion and seawater-resistant construction material. Low permeability. Highly stressed parts such as bevel gears, valves, worm wheels, fittings, hydraulic components, aviation industry. |